Table 3. Properties of Some Die Attach Adhesives from Ablestik

 

 

Adhesive Type

Conductivity

Cure Time (min)

Modulus (MPa)

Tg (șC)

Viscosity (cps)

Work Life (hrs)

ABLEBOND 16-1LV

Paste

Electrically conductive

30

N/A

N/A

N/A

2

ABLEBOND 2000B

Paste

Electrically conductive

45

2800

N/A

8700

24

ABLEBOND 2025

Paste

Electrically insulating

15

720

N/A

10500

24

ABLEBOND 3003

Paste

Thermally conductive

150

4000

49

30000

10

ABLEBOND 3230

Paste

Electrically conductive

15

2900

37

9000

24

ABLEBOND 826-1DS

Paste

Electrically conductive

30

5300

67

19000

24

ABLEBOND 8322A

Paste

Electrically conductive

1

1630

30

9000

24

ABLEBOND 8340A

Paste

Electrically conductive

15

910

25

9400

24

ABLEBOND 8360

Paste

Electrically conductive

60

4980

88

8000

20

ABLEBOND 8361HE

Paste

Electrically conductive

30

N/A

N/A

8500

24

ABLEBOND 8361J

Paste

Electrically conductive

90

2870

40

9400

24

ABLEBOND 8385

Paste

Electrically conductive

5

200000

14

9500

6

ABLEBOND 8390A

Paste

Electrically conductive

1

2300

53

9600

24

ABLEBOND 8390C

Paste

Electrically conductive

4

1800

19

9500

16

ABLEBOND 84-3J

Paste

Electrically insulating

60

6100

87

20000

336

ABLEBOND 84-3MVB

Paste

Non-conductive

120

6200

80

31000

48

ABLEBOND 8509

Paste

Electrically conductive

45

3800

40

8700

24

ABLEBOND 8510AA

Paste

Electrically conductive

15

2760

38

8800

N/A

ABLEBOND 8515

Paste

Non-conductive

15

1300

39

11500

24

ABLEBOND MA-2

Paste

Electrically conductive

30

N/A

108

N/A

24

ABLEBOND MC723

Paste

Electrically insulating

15

7000

75

55000

16

ABLEBOND OA-1S

Paste

Non-conductive

135

1100

60

325

10

ABLEFILL JM8806

Paste

Electrically insulating

90

8000

144

6000

24

ABLEFILL UF8802B

Paste

Electrically insulating

90

10000

142

7500

24

ABLEFILL UF8807

Paste

Electrically insulating

30

10000

147

17000

8

ABLETHERM 2600BT

Paste

Electrically conductive

15

4300

41

9300

24

UF8806LP

Paste

Non-conductive

90

1

144

6500

24

ABLEBOND 2025D

Paste

Electrically insulating

15

640

42

12200

24

ABLEBOND 2100A

Paste

Electrically conductive

15

1500

60

9000

24

ABLEBOND 2200

Paste

Electrically conductive

30

166

-15

9000

24

ABLEBOND 3902

Paste

Electrically conductive

60

2800

N/A

20000

2

ABLEBOND 71-1

Paste

Electrically conductive

60

3400

240

14000

N/A

ABLEBOND 789-3

Paste

Non-Conductive

30

N/A

126

N/A

N/A

ABLEBOND 8207

Paste

Electrically conductive

60

4800

63

11000

24

ABLEBOND 8340

Paste

Electrically conductive

30

710

25

9000

24

ABLEBOND 8390

Paste

Electrically conductive

2

4650

73

8800

48

ABLEBOND 84-1LMISR4

Paste

Electrically conductive

60

3940

120

8000

18

ABLEBOND 84-3MV

Paste

Non-Conductive

60

N/A

N/A

29000

N/A

ABLEBOND 868-7

Paste

Non-Conductive

15

N/A

N/A

N/A

1

ABLEBOND 8806

Paste

Non-Conductive

10

N/A

240

60000

N/A

ABLEBOND 965-1L

Paste

Electrically conductive

60

4800

85

12000

24

ABLEBOND 967-3

Paste

Thermally conductive

5

N/A

85

7000

48

ABLEBOND 979-1A

Paste

Electrically conductive

1

3800

193

15000

24

ABLEBOND 9902

Paste

Thermally conductive

240

N/A

N/A

20000

3

ABLEBOND BF-2

Paste

Non-conductive

60

3800

98

25000

48

ABLEBOND BF-4

Paste

Non-conductive

30

N/A

94

22500

24

ABLEBOND JM1032A

Paste

Electrically conductive

5

1000

73

6500

24

ABLEBOND JM2500

Paste

Electrically conductive

120

400

60

4500

12

ABLEBOND JM7000LV

Paste

Electrically conductive

30

10000

240

5000

8

ABLEBOND JM7000NC

Paste

Non-conductive

N/A

10500

220

8000

8

ABLEBOND JM7800

Paste

Electrically conductive

30

5000

184

11000

8

ABLEBOND LS-1

Paste

Non-conductive

30

2900

90

54500

24

ABLEBOND MA-1

Paste

Electrically conductive

30

700000

78

15000

24

ABLEFILL JM8801

Paste

Electrically insulating

90

10000

146

6000

24

ABLELUX LS-2

Paste

Non-conductive

60

2600

50

30000

24

ABLETHERM 2600K

Paste

Thermally conductive

45

3670

68

8100

24

ABLETHERM 3185

Paste

Electrically conductive

150

285

39

44000

16

   

<Back to Page 1 - Die Attach Materials>    <Back to Page 2 - D/A Alloys from SPM and Loctite>

  

 

   

See Also:  Semiconductor Materials;   Die Attach Process;   Semiconductor Manufacturing

            

HOME

                 

Copyright © 2005. SiliconFarEast.com. All Rights Reserved.